Tuotteen kuvaus
In principle, a prepolymer could be formed by reacting diisocyanates with an excess of polyol to produce a polyol functional prepolymer with urethane functionality at its center, but this is not practiced commercially and the term "prepolymer" is always used to refer to polyols terminated with isocyanate functionality. The excess isocyanate is required to prevent molecular weight growth caused by opportunistic chain extension of unreacted polyol reacting with the isocyanate-terminated prepolymer. In practice, chain extension always occurs but can be limited by increasing the ratio of isocyanate to hydroxyl functionality. A true "prepolymer" in this regard would then distill the excess isocyanate from the product. In the case where the excess isocyanate is left in the product, this is referred to as a "quasi-prepolymer". In practice, quasi-prepolymer refers to systems with relatively high levels of free isocyanate (>12%), kun taas esipolymeeri viittaa järjestelmiin, joissa on vähän vapaita isosyanaatteja (<12%). Overall, over 400 million pounds a year of prepolymer is used commercially for many applications where the advantages of prepolymers can be realized.
Tämä kvasi-MDI-esteripohjainen polyuretaaniesipolymeeri koostuu kolmesta komponentista A/B/C. Komponentti A on Quasi-MDI polyesteriesipolymeeri, joka päätyi isosynaattiin, komponentti B on polyesteripolyoli, komponentti C on 1,4BDO.
Sen näennäiset esipolymeerijärjestelmät voivat tarjota tiettyjä etuja tavanomaisiin täysesipolymeereihin verrattuna tarjoamalla alhaisemman viskositeetin esipolymeerejä ja kovetteita, alhaisemman materiaalin lämpötilan prosessointia varten, monikovuisia elastomeerejä samalla järjestelmällä sekä parempaa ympäristö- ja terveydenhuoltoa.
Suurin etu on lyhyt irrotusaika, mikä mahdollistaa tuottavuuden lisäämisen.
Etu
• Erinomaiset mekaaniset ominaisuudet
• Säädettävä reaktiivisuus eli katalyytin ja seossuhteen valinta
• Soveltuu erittäin suurten osien valamiseen
• Elinkelpoisia vaihtoehtoja järjestelmille, joihin saattaa kohdistua sääntelyrajoituksia
• Pienempi energiankulutus lisää kestävyyttä
Quasi-MDI-esteripohjaiset järjestelmät tarjoavat erinomaisen kulutuksen ja repeytymisen kestävyyden sekä erinomaisen kemikaalien, kuten hiilivedyt, öljyt ja liuottimet, kestävyyden. Nämä järjestelmät ovat ihanteellinen valinta sovelluksiin, kuten seuloihin, kaaviniin, sioihin, betoniteriin, levyihin ja tärymaljoihin.
Tyypilliset indikaattorit:
|
Tuote |
BQ3516-B |
BQ3516-A |
BQ3516-C |
|||||
|
NCO-pitoisuus/% |
16.5±0.2 |
- |
- |
|||||
|
Käyttölämpötila/aste |
45 |
70 |
45 |
|||||
|
Viskositeetti MPa-s |
700 |
730 |
30 |
|||||
|
Esipolymeeri |
BQ3516-B |
|||||||
|
Ketjun jatke |
BQ3516-A+BQ3516-C |
|||||||
|
Kovuus/Shore A |
55 |
60 |
65 |
70 |
75 |
80 |
85 |
90 |
|
BQ3516-B (suhde, painon mukaan) |
100 |
100 |
100 |
100 |
100 |
100 |
100 |
100 |
|
BQ3516-A (suhde, painon mukaan) |
380 |
180 |
160 |
130 |
110 |
100 |
80 |
60 |
|
BQ3516-C (suhde, painon mukaan) |
0 |
9.1 |
10 |
11.4 |
12.3 |
12.7 |
13.6 |
14.5 |
|
Katalyytti/kokonaispaino/(A+B+C)(%) |
0.4 |
0.4 |
0.4 |
0.4 |
0.3 |
0.3 |
0.3 |
0.3 |
|
Muotin lämpötila/aste |
100 |
|||||||
|
Geelimisaika/min |
5 |
5 |
5 |
5 |
5 |
4 |
4 |
4 |
|
Irrotusaika/min |
50 |
35 |
35 |
30 |
30 |
30 |
30 |
30 |
|
Jälkikovetusaika (100 astetta)/h |
16 |
|||||||
Fysikaaliset ominaisuudet
|
Kovuus/Shore A |
55 |
60 |
65 |
70 |
75 |
80 |
85 |
90 |
|
Vetolujuus/MPa |
16 |
36 |
43 |
46 |
48 |
49 |
50 |
50 |
|
Murtovenymä/% |
950 |
600 |
550 |
550 |
550 |
550 |
500 |
500 |
|
100 % moduuli/MPa |
1.4 |
2.2 |
2.4 |
3.7 |
4.6 |
5.2 |
6.6 |
9.6 |
|
300 % moduuli/MPa |
1.5 |
4.2 |
5.2 |
7.2 |
11.4 |
11.1 |
14.6 |
19.2 |
|
Repäisylujuus (ilman Nickiä) / (KN/m) |
23 |
55 |
66 |
78 |
88 |
98 |
106 |
125 |
|
Repäisylujuus (nikin kanssa) / (KN/m) |
11 |
21 |
29 |
34 |
38 |
44 |
56 |
63 |
|
Rebound(23 astetta)/ % |
56 |
50 |
50 |
48 |
47 |
47 |
46 |
44 |
|
Kulutushäviö/mm³/(DIN) |
11 |
12 |
14 |
15 |
15 |
17 |
19 |
22 |
|
Puristussarja/%(22H/70 astetta) |
15 |
17 |
19 |
21 |
24 |
26 |
29 |
32 |
|
Ominaispaino (25 astetta) (g/cm³) |
1.17 |
1.18 |
1.19 |
1.19 |
1.2 |
1.21 |
1.22 |
1.22 |
Pakkaus
Tämä Quasi MDI POLYESTER -järjestelmä yleensä pakattu 200 kg / rautarumpu


Suositut Tagit: kvasi-mdi-esteripohjaiset polyuretaaniesipolymeerit valuelastomeerille, Kiina kvasi-mdi-esteripohjaiset polyuretaaniesipolymeerit valuelastomeerien valmistajille, toimittajille, tehtaalle